| Item | Issue | Solution | Benefits |
| Small cavity | Surface corroded & worn | Tool polished back to remove surface damage from corrosion rendering tool 50mm undersize on diameter. Plated to 25mm thickness with ENi. | Corrosion Problem Eliminated. Harder ENi coating improved wear resistance and deposit thickness brought tool back to required dimensions |
| Small injection moulding tools | Parts sticking on release | 15mm deposit of ENi, then polished | Extra lubricity of polished ENi deposit enabled parts to release easily. Problem ceased. |
| Large injection moulding tool | Severe corrosion through water channels | Clean out water channels and plate with 10-12mm ENi | ENi provided corrosion resistance through water channels improving down-time and maintenance of tool. |
| Foundry Tool | Guide pins wearing out | Machine guide pins to allow a 50mm deposit of ENi. Harden EN to 65 RC | Excellent wear characteristics of ENi extended life of pins enabling tool to remain in service up to 3 times longer than previous |